[{"data":1,"prerenderedAt":1023},["ShallowReactive",2],{"article-dyeing-tr-fabric":3},{"id":4,"tenant":5,"status":13,"source":14,"kind":15,"slug":16,"publishedAt":17,"title_th":18,"excerpt_th":19,"body_th":20,"seoTitle_th":18,"seoDescription_th":522,"keywords_th":523,"title_en":524,"excerpt_en":525,"body_en":526,"seoTitle_en":524,"seoDescription_en":997,"keywords_en":998,"cover":999,"coverUrl":1002,"coverAlt":1002,"bodyHtml_th":1019,"bodyHtml_en":1020,"updatedAt":1021,"createdAt":1022,"coverSrc":1013,"coverAltResolved":1001},45,{"id":6,"slug":7,"name":8,"domain":9,"deployHookEnv":10,"updatedAt":11,"createdAt":12},1,"boonchuay","Boonchuay Group","boonchuay.com","DEPLOY_HOOK_BOONCHUAY","2026-09-01T14:50:36.814Z","2026-09-01T13:03:54.063Z","published","cmp-ai","article","dyeing-tr-fabric","2026-11-16T20:37:58.437Z","ผ้า TR ย้อมอย่างไร: 2 เส้นใย 2 ระบบย้อม ให้ผ้ายูนิฟอร์ม","ผ้า TR ผืนเดียวมีเส้นใย 2 ชนิด — โพลีเอสเตอร์กับเรยอง — จึงต้องผ่านสีย้อม 2 ระบบก่อนจะเป็นสีเดียว ผลลัพธ์คือผ้านุ่ม เรียบ ทรงตัวดี เหมาะกับงานยูนิฟอร์ม",{"root":21},{"type":22,"format":23,"indent":24,"version":6,"children":25,"direction":34},"root","",0,[26,35,56,60,72,105,109,124,156,160,210,214,222,266,270,308,312,316,357,361,373,407,411,417,421,427,433,439,445,449,475,479],{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":29,"direction":34},"h2","heading",[30],{"mode":31,"text":32,"type":33,"style":23,"detail":24,"format":24,"version":6},"normal","คำตอบสั้น: ผ้า TR ย้อมอย่างไร","text","ltr",{"type":36,"format":23,"indent":24,"version":6,"children":37,"direction":34,"textStyle":23,"textFormat":24},"paragraph",[38,40,42,44,46,48,50,52,54],{"mode":31,"text":39,"type":33,"style":23,"detail":24,"format":24,"version":6},"ผ้า TR (polyester-rayon) คือผ้าผสมระหว่าง",{"mode":31,"text":41,"type":33,"style":23,"detail":24,"format":6,"version":6},"โพลีเอสเตอร์กับเรยอง (วิสโคส)",{"mode":31,"text":43,"type":33,"style":23,"detail":24,"format":24,"version":6}," ซึ่งเป็นเส้นใยเซลลูโลสที่นำกลับมาผลิตใหม่จากเยื่อไม้ — เพราะผืนเดียวมีเส้นใย 2 ชนิด จึง",{"mode":31,"text":45,"type":33,"style":23,"detail":24,"format":6,"version":6},"ย้อมด้วยสีย้อมกลุ่มเดียวไม่ได้",{"mode":31,"text":47,"type":33,"style":23,"detail":24,"format":24,"version":6},": โพลีเอสเตอร์ใช้สีย้อมดิสเปอร์ส (ย้อมด้วยความร้อนสูง) ส่วนเรยองใช้สีย้อมรีแอคทีฟ (หรือ vat) ที่อุณหภูมิต่ำกว่า การย้อม 2 ระบบเรียงลำดับนี้เองที่ทำให้ผ้า TR มีทั้ง",{"mode":31,"text":49,"type":33,"style":23,"detail":24,"format":6,"version":6},"ความนุ่มและทิ้งตัว (drape) ของเรยอง",{"mode":31,"text":51,"type":33,"style":23,"detail":24,"format":24,"version":6}," และ",{"mode":31,"text":53,"type":33,"style":23,"detail":24,"format":6,"version":6},"ทรงตัว ไม่หดง่ายของโพลีเอสเตอร์",{"mode":31,"text":55,"type":33,"style":23,"detail":24,"format":24,"version":6}," ในผืนเดียว",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":57,"direction":34},[58],{"mode":31,"text":59,"type":33,"style":23,"detail":24,"format":24,"version":6},"ผ้า TR คืออะไร ต่างจากผ้า TC อย่างไร",{"type":36,"format":23,"indent":24,"version":6,"children":61,"direction":34,"textStyle":23,"textFormat":24},[62,64,66,68,70],{"mode":31,"text":63,"type":33,"style":23,"detail":24,"format":24,"version":6},"TR คือผ้าผสม",{"mode":31,"text":65,"type":33,"style":23,"detail":24,"format":6,"version":6},"โพลีเอสเตอร์ (T) กับเรยอง\u002Fวิสโคส (R)",{"mode":31,"text":67,"type":33,"style":23,"detail":24,"format":24,"version":6}," — โครงสร้างการย้อมเหมือนผ้า TC ทุกประการ (2 ใย 2 สีย้อม) แต่เปลี่ยนเส้นใยด้านเซลลูโลสจาก",{"mode":31,"text":69,"type":33,"style":23,"detail":24,"format":6,"version":6},"ฝ้ายเป็นเรยอง",{"mode":31,"text":71,"type":33,"style":23,"detail":24,"format":24,"version":6}," ผลที่ตามมาคือ:",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":75,"listType":104,"direction":34},"ul","list",[76,83,90,97],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":78,"direction":34},"listitem",[79,81],{"mode":31,"text":80,"type":33,"style":23,"detail":24,"format":6,"version":6},"เรยองดูดน้ำและให้ความนุ่มมากกว่าฝ้าย",{"mode":31,"text":82,"type":33,"style":23,"detail":24,"format":24,"version":6}," — เนื้อผ้าจึงนุ่ม เรียบ และทิ้งตัว (drape) กว่า TC",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":85,"direction":34},2,[86,88],{"mode":31,"text":87,"type":33,"style":23,"detail":24,"format":6,"version":6},"เรยองมีความแข็งแรงต่ำเมื่อเปียก",{"mode":31,"text":89,"type":33,"style":23,"detail":24,"format":24,"version":6}," (wet strength ต่ำ) — ใช้น้ำหนักและความทนในการซัก-รีดที่เบากว่า TC เล็กน้อย",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":92,"direction":34},3,[93,95],{"mode":31,"text":94,"type":33,"style":23,"detail":24,"format":6,"version":6},"เรยองหดตัวได้ง่ายกว่าฝ้าย",{"mode":31,"text":96,"type":33,"style":23,"detail":24,"format":24,"version":6}," — ต้องอาศัยขั้นตอนหลังการย้อม (sanforize) คุมขนาดให้แน่นกว่า",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":99,"direction":34},4,[100,102],{"mode":31,"text":101,"type":33,"style":23,"detail":24,"format":6,"version":6},"เรยองติดสีได้สดใส",{"mode":31,"text":103,"type":33,"style":23,"detail":24,"format":24,"version":6}," (amorphous region มาก) — เฉดสีจึงลึกและสดใส","bullet",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":106,"direction":34},[107],{"mode":31,"text":108,"type":33,"style":23,"detail":24,"format":24,"version":6},"ทำไมผ้า TR ต้องย้อม 2 ระบบ",{"type":36,"format":23,"indent":24,"version":6,"children":110,"direction":34,"textStyle":23,"textFormat":24},[111,113,122],{"mode":31,"text":112,"type":33,"style":23,"detail":24,"format":24,"version":6},"ผืนเดียวมีเส้นใย 2 ชนิดที่เคมีต่างกัน จึงต้องใช้สีย้อมคนละกลุ่ม (กลไกเดียวกับผ้า TC — อ่านเพิ่มใน ",{"type":114,"fields":115,"format":23,"indent":24,"version":91,"children":119,"direction":34},"link",{"url":116,"newTab":117,"linkType":118},"\u002Fth\u002Farticles\u002Fdyeing-tc-fabric\u002F",false,"custom",[120],{"mode":31,"text":121,"type":33,"style":23,"detail":24,"format":24,"version":6},"ผ้า TC ย้อมอย่างไร",{"mode":31,"text":123,"type":33,"style":23,"detail":24,"format":24,"version":6},"):",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":125,"listType":104,"direction":34},[126,136,148],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":127,"direction":34},[128,130,132,134],{"mode":31,"text":129,"type":33,"style":23,"detail":24,"format":6,"version":6},"โพลีเอสเตอร์",{"mode":31,"text":131,"type":33,"style":23,"detail":24,"format":24,"version":6}," — ไม่ดูดน้ำ ใช้",{"mode":31,"text":133,"type":33,"style":23,"detail":24,"format":6,"version":6},"สีย้อมดิสเปอร์ส",{"mode":31,"text":135,"type":33,"style":23,"detail":24,"format":24,"version":6},": โมเลกุลเล็กซึมเข้าเส้นใยที่อุณหภูมิสูง (HTHP jet ราว 130°C หรือแบบต่อเนื่อง thermosol 180–220°C) — ดิสเปอร์สยึดกับโพลีเอสเตอร์เป็นหลัก ไม่ติดเส้นใยเซลลูโลส",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":137,"direction":34},[138,140,142,144,146],{"mode":31,"text":139,"type":33,"style":23,"detail":24,"format":6,"version":6},"เรยอง (เซลลูโลส)",{"mode":31,"text":141,"type":33,"style":23,"detail":24,"format":24,"version":6}," — ใช้",{"mode":31,"text":143,"type":33,"style":23,"detail":24,"format":6,"version":6},"สีย้อมรีแอคทีฟ",{"mode":31,"text":145,"type":33,"style":23,"detail":24,"format":24,"version":6}," (สร้างพันธะเคมีกับเซลลูโลสที่ 60–80°C แล้วตรึงด้วยด่าง) หรือ",{"mode":31,"text":147,"type":33,"style":23,"detail":24,"format":6,"version":6},"vat dye",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":149,"direction":34},[150,152,154],{"mode":31,"text":151,"type":33,"style":23,"detail":24,"format":24,"version":6},"ลำดับต้อง",{"mode":31,"text":153,"type":33,"style":23,"detail":24,"format":6,"version":6},"ย้อมโพลีเอสเตอร์ก่อน",{"mode":31,"text":155,"type":33,"style":23,"detail":24,"format":24,"version":6}," เพราะขั้นตอนดิสเปอร์สใช้ความร้อนสูงมาก — ถ้าย้อมรีแอคทีฟก่อน ความร้อนจากขั้นดิสเปอร์สจะทำลายสีย้อมรีแอคทีฟ",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":157,"direction":34},[158],{"mode":31,"text":159,"type":33,"style":23,"detail":24,"format":24,"version":6},"ขั้นตอนการย้อมผ้า TR",{"tag":161,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":162,"listType":209,"direction":34},"ol",[163,173,179,185,191,198],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":164,"direction":34},[165,167,169,171],{"mode":31,"text":166,"type":33,"style":23,"detail":24,"format":6,"version":6},"เตรียมผ้า (pretreatment)",{"mode":31,"text":168,"type":33,"style":23,"detail":24,"format":24,"version":6}," — ฟอกแป้ง (desizing) ต้มฟอก (scouring) และฟอกขาวตามความจำเป็น; โพลีเอสเตอร์ต้อง",{"mode":31,"text":170,"type":33,"style":23,"detail":24,"format":6,"version":6},"รีดร้อน (heat set)",{"mode":31,"text":172,"type":33,"style":23,"detail":24,"format":24,"version":6}," ก่อน ไม่งั้นเส้นใยจะคลายตัวทำให้ผ้าเสียทรง",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":174,"direction":34},[175,177],{"mode":31,"text":176,"type":33,"style":23,"detail":24,"format":6,"version":6},"ย้อมโพลีเอสเตอร์",{"mode":31,"text":178,"type":33,"style":23,"detail":24,"format":24,"version":6}," — สีย้อมดิสเปอร์ส ใน pH กรดอ่อน (ราว 5–6) ใช้น้ำยากระจายสีและสาร levelling ในเครื่อง jet (HTHP) หรือแบบต่อเนื่อง thermosol (จุ่มสีแล้วอบแห้ง 180–220°C)",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":180,"direction":34},[181,183],{"mode":31,"text":182,"type":33,"style":23,"detail":24,"format":6,"version":6},"ขจัดสีดิสเปอร์สที่เปื้อนเรยอง (reduction clearing)",{"mode":31,"text":184,"type":33,"style":23,"detail":24,"format":24,"version":6}," — ล้างสีย้อมดิสเปอร์สที่เกาะเส้นใยเรยองออกก่อนย้อมขั้นถัดไป (ใช้เมื่อเฉดทำให้ด้านเรยองติดสี)",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":186,"direction":34},[187,189],{"mode":31,"text":188,"type":33,"style":23,"detail":24,"format":6,"version":6},"ย้อมเรยอง",{"mode":31,"text":190,"type":33,"style":23,"detail":24,"format":24,"version":6}," — สีย้อมรีแอคทีฟ (jet หรือ pad-batch) ที่ 60–80°C แล้วตรึงด้วยด่าง",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":193,"direction":34},5,[194,196],{"mode":31,"text":195,"type":33,"style":23,"detail":24,"format":6,"version":6},"รีดสี (soaping) และล้าง",{"mode":31,"text":197,"type":33,"style":23,"detail":24,"format":24,"version":6}," — ขจัดสีย้อมที่ยังไม่ตรึงออกด้วยความร้อนพร้อมผงซักฟอก แล้วล้างและอบแห้ง",{"type":77,"value":199,"format":23,"indent":24,"version":6,"children":200,"direction":34},6,[201,203,205,207],{"mode":31,"text":202,"type":33,"style":23,"detail":24,"format":6,"version":6},"หลังการย้อม (finishing)",{"mode":31,"text":204,"type":33,"style":23,"detail":24,"format":24,"version":6}," — โดยเฉพาะ",{"mode":31,"text":206,"type":33,"style":23,"detail":24,"format":6,"version":6},"กันหด (sanforizing)",{"mode":31,"text":208,"type":33,"style":23,"detail":24,"format":24,"version":6}," เพื่อให้ผ้ายืนยันทรงสุดท้าย ซึ่งสำคัญมากสำหรับ TR","number",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":211,"direction":34},[212],{"mode":31,"text":213,"type":33,"style":23,"detail":24,"format":24,"version":6},"ทำไมผ้า TR ถึงเหมาะกับการทำยูนิฟอร์ม",{"type":36,"format":23,"indent":24,"version":6,"children":215,"direction":34,"textStyle":23,"textFormat":24},[216,218,220],{"mode":31,"text":217,"type":33,"style":23,"detail":24,"format":24,"version":6},"ยูนิฟอร์มต้องการผ้าที่",{"mode":31,"text":219,"type":33,"style":23,"detail":24,"format":6,"version":6},"ดูเรียบร้อย นุ่ม สวมใส่สบาย และทนต่อการซัก-รีดบ่อย",{"mode":31,"text":221,"type":33,"style":23,"detail":24,"format":24,"version":6}," — TR ตอบครบ:",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":223,"listType":104,"direction":34},[224,237,246,258],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":225,"direction":34},[226,228,230,232,233,235],{"mode":31,"text":227,"type":33,"style":23,"detail":24,"format":6,"version":6},"เรยอง",{"mode":31,"text":229,"type":33,"style":23,"detail":24,"format":24,"version":6}," ให้ความ",{"mode":31,"text":231,"type":33,"style":23,"detail":24,"format":6,"version":6},"นุ่ม เรียบ ทิ้งตัว",{"mode":31,"text":51,"type":33,"style":23,"detail":24,"format":24,"version":6},{"mode":31,"text":234,"type":33,"style":23,"detail":24,"format":6,"version":6},"ดูดซับเหงื่อ",{"mode":31,"text":236,"type":33,"style":23,"detail":24,"format":24,"version":6}," (moisture regain สูงกว่าฝ้าย) — สวมใส่สบาย",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":238,"direction":34},[239,240,241,243,244],{"mode":31,"text":129,"type":33,"style":23,"detail":24,"format":6,"version":6},{"mode":31,"text":229,"type":33,"style":23,"detail":24,"format":24,"version":6},{"mode":31,"text":242,"type":33,"style":23,"detail":24,"format":6,"version":6},"ทรงตัว ไม่หดง่าย ไม่ยับง่าย",{"mode":31,"text":51,"type":33,"style":23,"detail":24,"format":24,"version":6},{"mode":31,"text":245,"type":33,"style":23,"detail":24,"format":6,"version":6},"รีดง่าย",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":247,"direction":34},[248,250,252,254,256],{"mode":31,"text":249,"type":33,"style":23,"detail":24,"format":24,"version":6},"ผสมกันจึงได้ผ้ายูนิฟอร์มที่",{"mode":31,"text":251,"type":33,"style":23,"detail":24,"format":6,"version":6},"นุ่มกว่า TC",{"mode":31,"text":253,"type":33,"style":23,"detail":24,"format":24,"version":6}," แต่ยัง",{"mode":31,"text":255,"type":33,"style":23,"detail":24,"format":6,"version":6},"ทนการซักบ่อย",{"mode":31,"text":257,"type":33,"style":23,"detail":24,"format":24,"version":6}," — เหมาะกับชุดสำนักงาน โรงแรม และชุดทำงาน",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":259,"direction":34},[260,262,264],{"mode":31,"text":261,"type":33,"style":23,"detail":24,"format":24,"version":6},"เป็นผ้า",{"mode":31,"text":263,"type":33,"style":23,"detail":24,"format":6,"version":6},"น้ำหนักมาตรฐานไปจนถึงหนา",{"mode":31,"text":265,"type":33,"style":23,"detail":24,"format":24,"version":6}," (ไม่ใช่ผ้าบางเบา) ซึ่งเหมาะกับงานยูนิฟอร์มที่ต้องการความเรียบร้อย",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":267,"direction":34},[268],{"mode":31,"text":269,"type":33,"style":23,"detail":24,"format":24,"version":6},"เปรียบเทียบผ้า TR vs TC",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":271,"listType":104,"direction":34},[272,278,284,290,296,302],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":273,"direction":34},[274,276],{"mode":31,"text":275,"type":33,"style":23,"detail":24,"format":6,"version":6},"เส้นใยด้านเซลลูโลส",{"mode":31,"text":277,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR = เรยอง (วิสโคส) \u002F TC = ฝ้าย",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":279,"direction":34},[280,282],{"mode":31,"text":281,"type":33,"style":23,"detail":24,"format":6,"version":6},"สัมผัส (hand)",{"mode":31,"text":283,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR นุ่มและเรียบกว่า TC \u002F TC หนาและแข็งแรงกว่า",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":285,"direction":34},[286,288],{"mode":31,"text":287,"type":33,"style":23,"detail":24,"format":6,"version":6},"การดูดซับ",{"mode":31,"text":289,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR (เรยอง) ดูดน้ำและเหงื่อมากกว่าฝ้ายใน TC",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":291,"direction":34},[292,294],{"mode":31,"text":293,"type":33,"style":23,"detail":24,"format":6,"version":6},"ความแข็งแรงเมื่อเปียก (wet strength)",{"mode":31,"text":295,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR ต่ำกว่า TC เล็กน้อย — เพราะเรยองอ่อนกว่าฝ้ายเมื่อเปียก",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":297,"direction":34},[298,300],{"mode":31,"text":299,"type":33,"style":23,"detail":24,"format":6,"version":6},"การหดตัว",{"mode":31,"text":301,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR (เรยอง) หดง่ายกว่า — ต้อง sanforize คุมแน่นกว่า",{"type":77,"value":199,"format":23,"indent":24,"version":6,"children":303,"direction":34},[304,306],{"mode":31,"text":305,"type":33,"style":23,"detail":24,"format":6,"version":6},"การใช้งานหลัก",{"mode":31,"text":307,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR = ยูนิฟอร์มที่ต้องการความนุ่มเรียบร้อย \u002F TC = ยูนิฟอร์มที่ต้องการความทนและแข็งแรง",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":309,"direction":34},[310],{"mode":31,"text":311,"type":33,"style":23,"detail":24,"format":24,"version":6},"โรงงานย้อมผ้าคุมคุณภาพผ้า TR อย่างไร",{"type":36,"format":23,"indent":24,"version":6,"children":313,"direction":34,"textStyle":23,"textFormat":24},[314],{"mode":31,"text":315,"type":33,"style":23,"detail":24,"format":24,"version":6},"เพราะ TR มีเส้นใย 2 ชนิด ควบคุมให้ได้สีเดียวและทรงตัวดีต้องอาศัย:",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":317,"listType":104,"direction":34},[318,324,330,336,340,346,352],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":319,"direction":34},[320,322],{"mode":31,"text":321,"type":33,"style":23,"detail":24,"format":6,"version":6},"ห้องสี (colour lab)",{"mode":31,"text":323,"type":33,"style":23,"detail":24,"format":24,"version":6}," — สเปกโทรโฟโตมิเตอร์ + ห้องตรวจสีหลายแหล่งแสง สำหรับทำ swatch (lab dip)",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":325,"direction":34},[326,328],{"mode":31,"text":327,"type":33,"style":23,"detail":24,"format":6,"version":6},"ย้อมตัวอย่าง (lab dyeing) ที่จำลอง process ผลิตจริง",{"mode":31,"text":329,"type":33,"style":23,"detail":24,"format":24,"version":6}," (batch และ continuous)",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":331,"direction":34},[332,334],{"mode":31,"text":333,"type":33,"style":23,"detail":24,"format":6,"version":6},"standard sample ที่ buyer ลงนาม",{"mode":31,"text":335,"type":33,"style":23,"detail":24,"format":24,"version":6}," เก็บไว้เทียบข้ามออเดอร์",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":337,"direction":34},[338],{"mode":31,"text":339,"type":33,"style":23,"detail":24,"format":6,"version":6},"สูตรสีและ process conditions ที่ล็อกให้คงที่",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":341,"direction":34},[342,344],{"mode":31,"text":343,"type":33,"style":23,"detail":24,"format":6,"version":6},"ค่า ΔE จากสเปกโทรโฟโตมิเตอร์",{"mode":31,"text":345,"type":33,"style":23,"detail":24,"format":24,"version":6}," วัดความต่างสีของทุกล็อตเทียบกับ standard",{"type":77,"value":199,"format":23,"indent":24,"version":6,"children":347,"direction":34},[348,350],{"mode":31,"text":349,"type":33,"style":23,"detail":24,"format":6,"version":6},"การทดสอบตามมาตรฐานที่ระบุวิธีและระดับ",{"mode":31,"text":351,"type":33,"style":23,"detail":24,"format":24,"version":6}," — เช่น ซัก (ISO 105-C06), สีติด (ISO 105-X12), แสง (ISO 105-B02), หดตัว (ISO 6330 \u002F AATCC 135)",{"type":77,"value":353,"format":23,"indent":24,"version":6,"children":354,"direction":34},7,[355],{"mode":31,"text":356,"type":33,"style":23,"detail":24,"format":24,"version":6},"รายงานคุณภาพระบบ 10 จุดทุกล็อต",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":358,"direction":34},[359],{"mode":31,"text":360,"type":33,"style":23,"detail":24,"format":24,"version":6},"บุญช่วยอุตสาหกรรม: รับย้อมผ้า TR",{"type":36,"format":23,"indent":24,"version":6,"children":362,"direction":34,"textStyle":23,"textFormat":24},[363,365,367,369,371],{"mode":31,"text":364,"type":33,"style":23,"detail":24,"format":24,"version":6},"บุญช่วยอุตสาหกรรม (BCI) คือโรงงานฟอกย้อมและตกแต่งผ้าที่มีประสบการณ์",{"mode":31,"text":366,"type":33,"style":23,"detail":24,"format":6,"version":6},"กว่า 60 ปี",{"mode":31,"text":368,"type":33,"style":23,"detail":24,"format":24,"version":6}," ที่จังหวัดนครปฐม — ",{"mode":31,"text":370,"type":33,"style":23,"detail":24,"format":6,"version":6},"รับย้อมผ้า",{"mode":31,"text":372,"type":33,"style":23,"detail":24,"format":24,"version":6}," กลุ่ม TR (โพลีเอสเตอร์-เรยอง) และ TC ซึ่งเป็นเส้นใยหลักของงานยูนิฟอร์ม:",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":374,"listType":104,"direction":34},[375,381,387,391,395,401],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":376,"direction":34},[377,379],{"mode":31,"text":378,"type":33,"style":23,"detail":24,"format":6,"version":6},"process ครบ",{"mode":31,"text":380,"type":33,"style":23,"detail":24,"format":24,"version":6}," — เตรียมผ้า (ฟอก\u002Fต้มฟอก), ย้อม, หลังการย้อม และห้องสี",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":382,"direction":34},[383,385],{"mode":31,"text":384,"type":33,"style":23,"detail":24,"format":6,"version":6},"เครื่องย้อมทั้ง batch (jet) และ continuous",{"mode":31,"text":386,"type":33,"style":23,"detail":24,"format":24,"version":6}," — continuous ของ BCI ครอบคลุมสีอ่อนถึงเข้ม เหมาะกับออเดอร์ผ้ายูนิฟอร์มระยะยาว",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":388,"direction":34},[389],{"mode":31,"text":390,"type":33,"style":23,"detail":24,"format":24,"version":6},"QC 3 จุด — ตรวจผ้าดิบก่อนย้อม ควบคุมระหว่างกระบวนการ และตรวจตอนบรรจุ พร้อมรายงานคุณภาพระบบ 10 จุด",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":392,"direction":34},[393],{"mode":31,"text":394,"type":33,"style":23,"detail":24,"format":6,"version":6},"ทดสอบตามมาตรฐาน ISO, JIS, AATCC, Daimaru",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":396,"direction":34},[397,399],{"mode":31,"text":398,"type":33,"style":23,"detail":24,"format":6,"version":6},"ใบรับรอง OEKO-TEX Standard 100",{"mode":31,"text":400,"type":33,"style":23,"detail":24,"format":24,"version":6}," — ไม่มีสารห้ามใช้ในผ้าสำเร็จ",{"type":77,"value":199,"format":23,"indent":24,"version":6,"children":402,"direction":34},[403,405],{"mode":31,"text":404,"type":33,"style":23,"detail":24,"format":6,"version":6},"MOQ เจรจาได้",{"mode":31,"text":406,"type":33,"style":23,"detail":24,"format":24,"version":6}," — ขึ้นกับ process, สี และขนาดออเดอร์",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":408,"direction":34},[409],{"mode":31,"text":410,"type":33,"style":23,"detail":24,"format":24,"version":6},"ถาม-ตอบ (FAQ)",{"type":36,"format":23,"indent":24,"version":6,"children":412,"direction":34,"textStyle":23,"textFormat":24},[413,415],{"mode":31,"text":414,"type":33,"style":23,"detail":24,"format":6,"version":6},"ถาม: ผ้า TR ย้อมด้วยสีย้อมกลุ่มเดียวได้ไหม?",{"mode":31,"text":416,"type":33,"style":23,"detail":24,"format":24,"version":6}," ตอบ: ไม่ได้ — โพลีเอสเตอร์ต้องใช้สีย้อมดิสเปอร์ส (ความร้อนสูง) ส่วนเรยองใช้สีย้อมรีแอคทีฟหรือ vat ย้อมด้วยกลุ่มเดียวอีกเส้นใยจึงไม่ติดสี",{"type":36,"format":23,"indent":24,"version":6,"children":418,"direction":34,"textStyle":23,"textFormat":24},[419],{"mode":31,"text":420,"type":33,"style":23,"detail":24,"format":24,"version":6},"ถาม: TR กับ TC ต่างกันตรงไหน และควรเลือกอะไร? ตอบ: TR ใช้เรยองแทนฝ้าย — นุ่ม เรียบ และดูดซับมากกว่า แต่ความแข็งแรงตอนเปียกต่ำกว่าเล็กน้อยและหดง่ายกว่า TC เหมาะกับงานที่ต้องการความทนแข็งแรง TR เหมาะกับงานที่ต้องการความนุ่มเรียบร้อย BCI ย้อมได้ทั้งสอง",{"type":36,"format":23,"indent":24,"version":6,"children":422,"direction":34,"textStyle":23,"textFormat":24},[423,425],{"mode":31,"text":424,"type":33,"style":23,"detail":24,"format":6,"version":6},"ถาม: ทำไมต้องย้อมโพลีเอสเตอร์ก่อนเรยอง?",{"mode":31,"text":426,"type":33,"style":23,"detail":24,"format":24,"version":6}," ตอบ: ขั้นตอนดิสเปอร์สใช้ความร้อนสูงมาก (130°C หรือ thermosol 180–220°C) ถ้าย้อมรีแอคทีฟก่อน ความร้อนนั้นจะทำลายสีย้อมรีแอคทีฟจึงต้องเรียงลำดับดิสเปอร์สก่อน",{"type":36,"format":23,"indent":24,"version":6,"children":428,"direction":34,"textStyle":23,"textFormat":24},[429,431],{"mode":31,"text":430,"type":33,"style":23,"detail":24,"format":6,"version":6},"ถาม: ทำไมผ้า TR ถึงหดตัว?",{"mode":31,"text":432,"type":33,"style":23,"detail":24,"format":24,"version":6}," ตอบ: เรยอง (วิสโคส) มีแนวโน้มหดตัวและเสียทรงได้ง่ายกว่าฝ้าย จึงต้องอาศัยขั้นตอนหลังการย้อม เช่น sanforizing เพื่อล็อกขนาดให้แน่นก่อนส่งมอบ",{"type":36,"format":23,"indent":24,"version":6,"children":434,"direction":34,"textStyle":23,"textFormat":24},[435,437],{"mode":31,"text":436,"type":33,"style":23,"detail":24,"format":6,"version":6},"ถาม: ผ้า TR เหมาะกับงานยูนิฟอร์มประเภทไหน?",{"mode":31,"text":438,"type":33,"style":23,"detail":24,"format":24,"version":6}," ตอบ: ชุดสำนักงาน ชุดโรงแรม และชุดทำงานที่เน้นความนุ่ม เรียบ และสวมใส่สบาย ในขณะที่ยังต้องทนต่อการซัก-รีดบ่อย — BCI ย้อม TR สำหรับงานกลุ่มนี้",{"type":36,"format":23,"indent":24,"version":6,"children":440,"direction":34,"textStyle":23,"textFormat":24},[441,443],{"mode":31,"text":442,"type":33,"style":23,"detail":24,"format":6,"version":6},"ถาม: จำนวนน้อยย้อม TR ได้ไหม?",{"mode":31,"text":444,"type":33,"style":23,"detail":24,"format":24,"version":6}," ตอบ: MOQ เจรจาได้ — ขึ้นกับ process, สี และขนาด ล็อตเล็กสามารถเดินเครื่อง batch (jet) ได้",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":446,"direction":34},[447],{"mode":31,"text":448,"type":33,"style":23,"detail":24,"format":24,"version":6},"คุยกับทีม BCI",{"type":36,"format":23,"indent":24,"version":6,"children":450,"direction":34,"textStyle":23,"textFormat":24},[451,453,459,461,467,469],{"mode":31,"text":452,"type":33,"style":23,"detail":24,"format":24,"version":6},"ดู ",{"type":114,"fields":454,"format":23,"indent":24,"version":91,"children":456,"direction":34},{"url":455,"newTab":117,"linkType":118},"\u002Fth\u002Ffabric-dyeing\u002F",[457],{"mode":31,"text":458,"type":33,"style":23,"detail":24,"format":24,"version":6},"รับย้อมผ้า TR จากโรงงานย้อมผ้า",{"mode":31,"text":460,"type":33,"style":23,"detail":24,"format":24,"version":6}," · ",{"type":114,"fields":462,"format":23,"indent":24,"version":91,"children":464,"direction":34},{"url":463,"newTab":117,"linkType":118},"\u002Fth\u002Funiform-fabrics\u002F",[465],{"mode":31,"text":466,"type":33,"style":23,"detail":24,"format":24,"version":6},"ผ้ายูนิฟอร์ม",{"mode":31,"text":468,"type":33,"style":23,"detail":24,"format":24,"version":6}," · หรือ ",{"type":114,"fields":470,"format":23,"indent":24,"version":91,"children":472,"direction":34},{"url":471,"newTab":117,"linkType":118},"\u002Fth\u002Fcontact-us\u002F",[473],{"mode":31,"text":474,"type":33,"style":23,"detail":24,"format":24,"version":6},"สอบถาม",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":476,"direction":34},[477],{"mode":31,"text":478,"type":33,"style":23,"detail":24,"format":24,"version":6},"แหล่งอ้างอิง",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":480,"listType":104,"direction":34},[481,490,498,506,514],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":482,"direction":34},[483],{"type":114,"fields":484,"format":23,"indent":24,"version":91,"children":487,"direction":34},{"url":485,"newTab":486,"linkType":118},"https:\u002F\u002Ftextilelearner.net\u002Fproperties-of-viscose-rayon\u002F",true,[488],{"mode":31,"text":489,"type":33,"style":23,"detail":24,"format":24,"version":6},"Physical, Chemical and Mechanical Properties of Viscose Rayon — Textile Learner",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":491,"direction":34},[492],{"type":114,"fields":493,"format":23,"indent":24,"version":91,"children":495,"direction":34},{"url":494,"newTab":486,"linkType":118},"https:\u002F\u002Fskychemi.com\u002Fdisperse-dye-exhaust-vs-continuous-dyeing\u002F",[496],{"mode":31,"text":497,"type":33,"style":23,"detail":24,"format":24,"version":6},"Disperse Dye Exhaust vs. Continuous Dyeing: A Process Guide for Polyester — Skychemi",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":499,"direction":34},[500],{"type":114,"fields":501,"format":23,"indent":24,"version":91,"children":503,"direction":34},{"url":502,"newTab":486,"linkType":118},"https:\u002F\u002Fdaiwaborayon.co.jp\u002Fenglish\u002Ffeatures",[504],{"mode":31,"text":505,"type":33,"style":23,"detail":24,"format":24,"version":6},"Characteristics of Viscose Rayon — Daiwabo Rayon Co., Ltd.",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":507,"direction":34},[508],{"type":114,"fields":509,"format":23,"indent":24,"version":91,"children":511,"direction":34},{"url":510,"newTab":486,"linkType":118},"https:\u002F\u002Fwww.aatcc.org\u002Fwp-content\u002Fuploads\u002Fgibson_121979_18.pdf",[512],{"mode":31,"text":513,"type":33,"style":23,"detail":24,"format":24,"version":6},"The Thermosol Story — Joseph W. Gibson Jr. (Olney Medal Address), AATCC",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":515,"direction":34},[516],{"type":114,"fields":517,"format":23,"indent":24,"version":91,"children":519,"direction":34},{"url":518,"newTab":486,"linkType":118},"https:\u002F\u002Fwww.aatcc.org\u002Ftesting\u002Fstandards",[520],{"mode":31,"text":521,"type":33,"style":23,"detail":24,"format":24,"version":6},"Standard Test Methods and Procedures — AATCC","ย้อมผ้า TR (โพลีเอสเตอร์-เรยอง) 2 ใย 2 ระบบ — ดิสเปอร์สให้โพลีเอสเตอร์ รีแอคทีฟให้เรยอง — ขั้นตอน จุดเด่น และเหตุผลที่ TR เหมาะกับยูนิฟอร์ม","ย้อมผ้า TR, ผ้า TR, โพลีเอสเตอร์-เรยอง, พอลิ-วิสโคส","How TR Fabric Is Dyed: 2 Fibres, 2 Dye Systems, One Shade","One TR fabric carries two fibres — polyester and rayon — so it takes two dye systems before it becomes one shade. The payoff: a softer, smoother, shape-stable uniform fabric.",{"root":527},{"type":22,"format":23,"indent":24,"version":6,"children":528,"direction":34},[529,533,561,565,577,603,607,618,649,653,699,703,711,757,761,799,803,807,847,851,863,897,901,907,911,917,923,929,935,939,961,965],{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":530,"direction":34},[531],{"mode":31,"text":532,"type":33,"style":23,"detail":24,"format":24,"version":6},"Short answer: how is TR fabric dyed",{"type":36,"format":23,"indent":24,"version":6,"children":534,"direction":34,"textStyle":23,"textFormat":24},[535,537,539,541,543,545,547,549,551,553,555,557,559],{"mode":31,"text":536,"type":33,"style":23,"detail":24,"format":24,"version":6},"TR (polyester-rayon) fabric is a blend of ",{"mode":31,"text":538,"type":33,"style":23,"detail":24,"format":6,"version":6},"polyester and rayon (viscose)",{"mode":31,"text":540,"type":33,"style":23,"detail":24,"format":24,"version":6}," — a regenerated cellulosic fibre made from wood pulp. Because one fabric carries two fibres, it ",{"mode":31,"text":542,"type":33,"style":23,"detail":24,"format":6,"version":6},"cannot be dyed with a single dye class",{"mode":31,"text":544,"type":33,"style":23,"detail":24,"format":24,"version":6},": the polyester takes ",{"mode":31,"text":546,"type":33,"style":23,"detail":24,"format":6,"version":6},"disperse dyes",{"mode":31,"text":548,"type":33,"style":23,"detail":24,"format":24,"version":6}," (dyed at high heat) and the rayon takes ",{"mode":31,"text":550,"type":33,"style":23,"detail":24,"format":6,"version":6},"reactive (or vat) dyes",{"mode":31,"text":552,"type":33,"style":23,"detail":24,"format":24,"version":6}," at a milder temperature. Running those two dye systems in sequence is what gives TR both the ",{"mode":31,"text":554,"type":33,"style":23,"detail":24,"format":6,"version":6},"softness and drape of rayon",{"mode":31,"text":556,"type":33,"style":23,"detail":24,"format":24,"version":6}," and the ",{"mode":31,"text":558,"type":33,"style":23,"detail":24,"format":6,"version":6},"shape retention and low shrinkage of polyester",{"mode":31,"text":560,"type":33,"style":23,"detail":24,"format":24,"version":6}," in a single fabric.",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":562,"direction":34},[563],{"mode":31,"text":564,"type":33,"style":23,"detail":24,"format":24,"version":6},"What TR is — and how it differs from TC",{"type":36,"format":23,"indent":24,"version":6,"children":566,"direction":34,"textStyle":23,"textFormat":24},[567,569,571,573,575],{"mode":31,"text":568,"type":33,"style":23,"detail":24,"format":24,"version":6},"TR is a blend of ",{"mode":31,"text":570,"type":33,"style":23,"detail":24,"format":6,"version":6},"polyester (T) and rayon\u002Fviscose (R)",{"mode":31,"text":572,"type":33,"style":23,"detail":24,"format":24,"version":6},". Its dyeing structure is identical to TC (two fibres, two dye classes), but it swaps the cellulosic fibre from ",{"mode":31,"text":574,"type":33,"style":23,"detail":24,"format":6,"version":6},"cotton to rayon",{"mode":31,"text":576,"type":33,"style":23,"detail":24,"format":24,"version":6},". The consequences:",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":578,"listType":104,"direction":34},[579,585,591,597],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":580,"direction":34},[581,583],{"mode":31,"text":582,"type":33,"style":23,"detail":24,"format":6,"version":6},"Rayon absorbs more water and is softer than cotton",{"mode":31,"text":584,"type":33,"style":23,"detail":24,"format":24,"version":6}," — so TR has a softer, smoother, more draping hand than TC",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":586,"direction":34},[587,589],{"mode":31,"text":588,"type":33,"style":23,"detail":24,"format":6,"version":6},"Rayon has lower wet strength",{"mode":31,"text":590,"type":33,"style":23,"detail":24,"format":24,"version":6}," — it handles slightly less well under heavy wash-and-wear than TC",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":592,"direction":34},[593,595],{"mode":31,"text":594,"type":33,"style":23,"detail":24,"format":6,"version":6},"Rayon shrinks more readily than cotton",{"mode":31,"text":596,"type":33,"style":23,"detail":24,"format":24,"version":6}," — so it needs tighter control in finishing (sanforizing)",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":598,"direction":34},[599,601],{"mode":31,"text":600,"type":33,"style":23,"detail":24,"format":6,"version":6},"Rayon takes dye brightly",{"mode":31,"text":602,"type":33,"style":23,"detail":24,"format":24,"version":6}," (more amorphous region) — so shades run deeper and more vivid",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":604,"direction":34},[605],{"mode":31,"text":606,"type":33,"style":23,"detail":24,"format":24,"version":6},"Why TR needs two dye systems",{"type":36,"format":23,"indent":24,"version":6,"children":608,"direction":34,"textStyle":23,"textFormat":24},[609,611,617],{"mode":31,"text":610,"type":33,"style":23,"detail":24,"format":24,"version":6},"One fabric, two chemically different fibres, so two dye classes are required (the same mechanism as TC — see ",{"type":114,"fields":612,"format":23,"indent":24,"version":91,"children":614,"direction":34},{"url":613,"newTab":117,"linkType":118},"\u002Farticles\u002Fdyeing-tc-fabric\u002F",[615],{"mode":31,"text":616,"type":33,"style":23,"detail":24,"format":24,"version":6},"How TC Fabric Is Dyed",{"mode":31,"text":123,"type":33,"style":23,"detail":24,"format":24,"version":6},{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":619,"listType":104,"direction":34},[620,629,641],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":621,"direction":34},[622,624,626,627],{"mode":31,"text":623,"type":33,"style":23,"detail":24,"format":6,"version":6},"Polyester",{"mode":31,"text":625,"type":33,"style":23,"detail":24,"format":24,"version":6}," — hydrophobic; takes ",{"mode":31,"text":546,"type":33,"style":23,"detail":24,"format":6,"version":6},{"mode":31,"text":628,"type":33,"style":23,"detail":24,"format":24,"version":6},", whose small molecules enter the fibre at high temperature (HTHP jet around 130°C, or continuous thermosol at 180–220°C) — disperse bonds to polyester mainly and not to cellulosic fibres",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":630,"direction":34},[631,633,635,637,639],{"mode":31,"text":632,"type":33,"style":23,"detail":24,"format":6,"version":6},"Rayon (cellulosic)",{"mode":31,"text":634,"type":33,"style":23,"detail":24,"format":24,"version":6}," — takes ",{"mode":31,"text":636,"type":33,"style":23,"detail":24,"format":6,"version":6},"reactive dyes",{"mode":31,"text":638,"type":33,"style":23,"detail":24,"format":24,"version":6}," (a chemical bond to cellulose at 60–80°C, fixed with alkali) or ",{"mode":31,"text":640,"type":33,"style":23,"detail":24,"format":6,"version":6},"vat dyes",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":642,"direction":34},[643,645,647],{"mode":31,"text":644,"type":33,"style":23,"detail":24,"format":24,"version":6},"The order matters: ",{"mode":31,"text":646,"type":33,"style":23,"detail":24,"format":6,"version":6},"polyester is dyed first",{"mode":31,"text":648,"type":33,"style":23,"detail":24,"format":24,"version":6},", because the disperse step uses very high heat — dyeing the reactive side first would destroy the reactive dyes",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":650,"direction":34},[651],{"mode":31,"text":652,"type":33,"style":23,"detail":24,"format":24,"version":6},"How TR fabric is dyed, step by step",{"tag":161,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":654,"listType":209,"direction":34},[655,665,671,677,683,689],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":656,"direction":34},[657,659,661,663],{"mode":31,"text":658,"type":33,"style":23,"detail":24,"format":6,"version":6},"Pretreatment",{"mode":31,"text":660,"type":33,"style":23,"detail":24,"format":24,"version":6}," — desizing, scouring, and bleaching where needed; the polyester is ",{"mode":31,"text":662,"type":33,"style":23,"detail":24,"format":6,"version":6},"heat-set",{"mode":31,"text":664,"type":33,"style":23,"detail":24,"format":24,"version":6}," first, or the fibre relaxes and the fabric loses its shape",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":666,"direction":34},[667,669],{"mode":31,"text":668,"type":33,"style":23,"detail":24,"format":6,"version":6},"Polyester dyeing",{"mode":31,"text":670,"type":33,"style":23,"detail":24,"format":24,"version":6}," — disperse dyes at mildly acidic pH (about 5–6) with a dispersing agent and a levelling agent, in a jet (HTHP) or by continuous thermosol (padding then dry heat at 180–220°C)",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":672,"direction":34},[673,675],{"mode":31,"text":674,"type":33,"style":23,"detail":24,"format":6,"version":6},"Reduction clearing",{"mode":31,"text":676,"type":33,"style":23,"detail":24,"format":24,"version":6}," — strips disperse-dye staining from the rayon side before the next step (used whenever the shade leaves the rayon stained)",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":678,"direction":34},[679,681],{"mode":31,"text":680,"type":33,"style":23,"detail":24,"format":6,"version":6},"Rayon dyeing",{"mode":31,"text":682,"type":33,"style":23,"detail":24,"format":24,"version":6}," — reactive dyes (jet or pad-batch) at 60–80°C, fixed with alkali",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":684,"direction":34},[685,687],{"mode":31,"text":686,"type":33,"style":23,"detail":24,"format":6,"version":6},"Soaping and washing",{"mode":31,"text":688,"type":33,"style":23,"detail":24,"format":24,"version":6}," — unreacted dye is washed out at heat with detergent, then rinse and dry",{"type":77,"value":199,"format":23,"indent":24,"version":6,"children":690,"direction":34},[691,693,695,697],{"mode":31,"text":692,"type":33,"style":23,"detail":24,"format":6,"version":6},"Finishing",{"mode":31,"text":694,"type":33,"style":23,"detail":24,"format":24,"version":6}," — especially ",{"mode":31,"text":696,"type":33,"style":23,"detail":24,"format":6,"version":6},"shrinkproofing (sanforizing)",{"mode":31,"text":698,"type":33,"style":23,"detail":24,"format":24,"version":6}," to lock in the final shape, which matters more for TR",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":700,"direction":34},[701],{"mode":31,"text":702,"type":33,"style":23,"detail":24,"format":24,"version":6},"Why TR is well suited to uniforms",{"type":36,"format":23,"indent":24,"version":6,"children":704,"direction":34,"textStyle":23,"textFormat":24},[705,707,709],{"mode":31,"text":706,"type":33,"style":23,"detail":24,"format":24,"version":6},"Uniforms need a fabric that ",{"mode":31,"text":708,"type":33,"style":23,"detail":24,"format":6,"version":6},"looks neat, feels soft, is comfortable, and stands up to frequent washing",{"mode":31,"text":710,"type":33,"style":23,"detail":24,"format":24,"version":6}," — TR delivers all of it:",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":712,"listType":104,"direction":34},[713,727,737,749],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":714,"direction":34},[715,717,719,721,723,725],{"mode":31,"text":716,"type":33,"style":23,"detail":24,"format":6,"version":6},"Rayon",{"mode":31,"text":718,"type":33,"style":23,"detail":24,"format":24,"version":6}," gives a ",{"mode":31,"text":720,"type":33,"style":23,"detail":24,"format":6,"version":6},"soft, smooth, draping hand",{"mode":31,"text":722,"type":33,"style":23,"detail":24,"format":24,"version":6}," and ",{"mode":31,"text":724,"type":33,"style":23,"detail":24,"format":6,"version":6},"good sweat absorbency",{"mode":31,"text":726,"type":33,"style":23,"detail":24,"format":24,"version":6}," (higher moisture regain than cotton) — comfortable to wear",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":728,"direction":34},[729,730,732,734,735],{"mode":31,"text":623,"type":33,"style":23,"detail":24,"format":6,"version":6},{"mode":31,"text":731,"type":33,"style":23,"detail":24,"format":24,"version":6}," gives ",{"mode":31,"text":733,"type":33,"style":23,"detail":24,"format":6,"version":6},"shape retention, low shrinkage, low wrinkling",{"mode":31,"text":722,"type":33,"style":23,"detail":24,"format":24,"version":6},{"mode":31,"text":736,"type":33,"style":23,"detail":24,"format":6,"version":6},"easy ironing",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":738,"direction":34},[739,741,743,745,747],{"mode":31,"text":740,"type":33,"style":23,"detail":24,"format":24,"version":6},"Combined, TR is a ",{"mode":31,"text":742,"type":33,"style":23,"detail":24,"format":6,"version":6},"softer uniform fabric than TC",{"mode":31,"text":744,"type":33,"style":23,"detail":24,"format":24,"version":6}," that still ",{"mode":31,"text":746,"type":33,"style":23,"detail":24,"format":6,"version":6},"holds up to repeated washing",{"mode":31,"text":748,"type":33,"style":23,"detail":24,"format":24,"version":6}," — a fit for office, hotel and work uniforms",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":750,"direction":34},[751,753,755],{"mode":31,"text":752,"type":33,"style":23,"detail":24,"format":24,"version":6},"It comes in ",{"mode":31,"text":754,"type":33,"style":23,"detail":24,"format":6,"version":6},"standard-to-heavier weights",{"mode":31,"text":756,"type":33,"style":23,"detail":24,"format":24,"version":6}," (not a lightweight fabric), which suits neat uniform work",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":758,"direction":34},[759],{"mode":31,"text":760,"type":33,"style":23,"detail":24,"format":24,"version":6},"TR vs TC, side by side",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":762,"listType":104,"direction":34},[763,769,775,781,787,793],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":764,"direction":34},[765,767],{"mode":31,"text":766,"type":33,"style":23,"detail":24,"format":6,"version":6},"Cellulosic fibre",{"mode":31,"text":768,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR = rayon (viscose) \u002F TC = cotton",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":770,"direction":34},[771,773],{"mode":31,"text":772,"type":33,"style":23,"detail":24,"format":6,"version":6},"Hand",{"mode":31,"text":774,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR is softer and smoother \u002F TC is fuller and firmer",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":776,"direction":34},[777,779],{"mode":31,"text":778,"type":33,"style":23,"detail":24,"format":6,"version":6},"Absorbency",{"mode":31,"text":780,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR (rayon) absorbs more water and sweat than the cotton in TC",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":782,"direction":34},[783,785],{"mode":31,"text":784,"type":33,"style":23,"detail":24,"format":6,"version":6},"Wet strength",{"mode":31,"text":786,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR is slightly lower than TC — rayon is weaker than cotton when wet",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":788,"direction":34},[789,791],{"mode":31,"text":790,"type":33,"style":23,"detail":24,"format":6,"version":6},"Shrinkage",{"mode":31,"text":792,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR (rayon) shrinks more readily — it needs tighter sanforizing control",{"type":77,"value":199,"format":23,"indent":24,"version":6,"children":794,"direction":34},[795,797],{"mode":31,"text":796,"type":33,"style":23,"detail":24,"format":6,"version":6},"Typical use",{"mode":31,"text":798,"type":33,"style":23,"detail":24,"format":24,"version":6},": TR = uniforms where a soft, neat hand is wanted \u002F TC = uniforms where durability and firmness are wanted",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":800,"direction":34},[801],{"mode":31,"text":802,"type":33,"style":23,"detail":24,"format":24,"version":6},"How a dyeing mill keeps TR quality consistent",{"type":36,"format":23,"indent":24,"version":6,"children":804,"direction":34,"textStyle":23,"textFormat":24},[805],{"mode":31,"text":806,"type":33,"style":23,"detail":24,"format":24,"version":6},"Because TR carries two fibres, holding one shade and a stable shape takes:",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":808,"listType":104,"direction":34},[809,815,821,827,831,837,843],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":810,"direction":34},[811,813],{"mode":31,"text":812,"type":33,"style":23,"detail":24,"format":6,"version":6},"A colour lab",{"mode":31,"text":814,"type":33,"style":23,"detail":24,"format":24,"version":6}," — spectrophotometer plus a multi-source light booth for lab dips",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":816,"direction":34},[817,819],{"mode":31,"text":818,"type":33,"style":23,"detail":24,"format":6,"version":6},"Lab dyeing that mirrors the production route",{"mode":31,"text":820,"type":33,"style":23,"detail":24,"format":24,"version":6}," (batch and continuous)",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":822,"direction":34},[823,825],{"mode":31,"text":824,"type":33,"style":23,"detail":24,"format":6,"version":6},"A buyer-signed standard sample",{"mode":31,"text":826,"type":33,"style":23,"detail":24,"format":24,"version":6}," held for inter-order comparison",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":828,"direction":34},[829],{"mode":31,"text":830,"type":33,"style":23,"detail":24,"format":6,"version":6},"A locked recipe and process conditions",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":832,"direction":34},[833,835],{"mode":31,"text":834,"type":33,"style":23,"detail":24,"format":6,"version":6},"ΔE from the spectrophotometer",{"mode":31,"text":836,"type":33,"style":23,"detail":24,"format":24,"version":6}," measuring every lot against the standard",{"type":77,"value":199,"format":23,"indent":24,"version":6,"children":838,"direction":34},[839,841],{"mode":31,"text":840,"type":33,"style":23,"detail":24,"format":6,"version":6},"Testing to named methods and levels",{"mode":31,"text":842,"type":33,"style":23,"detail":24,"format":24,"version":6}," — e.g. wash (ISO 105-C06), crocking (ISO 105-X12), light (ISO 105-B02), dimensional change (ISO 6330 \u002F AATCC 135)",{"type":77,"value":353,"format":23,"indent":24,"version":6,"children":844,"direction":34},[845],{"mode":31,"text":846,"type":33,"style":23,"detail":24,"format":24,"version":6},"A 10-point system quality report for every lot",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":848,"direction":34},[849],{"mode":31,"text":850,"type":33,"style":23,"detail":24,"format":24,"version":6},"Boonchuay Industrial (BCI): commission dyeing for TR",{"type":36,"format":23,"indent":24,"version":6,"children":852,"direction":34,"textStyle":23,"textFormat":24},[853,855,857,859,861],{"mode":31,"text":854,"type":33,"style":23,"detail":24,"format":24,"version":6},"BCI (Boonchuay Industrial) is a fabric dyeing and finishing mill with ",{"mode":31,"text":856,"type":33,"style":23,"detail":24,"format":6,"version":6},"over 60 years",{"mode":31,"text":858,"type":33,"style":23,"detail":24,"format":24,"version":6}," of experience in Nakhon Pathom, Thailand. It takes ",{"mode":31,"text":860,"type":33,"style":23,"detail":24,"format":6,"version":6},"TR (polyester-rayon) and TC",{"mode":31,"text":862,"type":33,"style":23,"detail":24,"format":24,"version":6}," — its core uniform fibres — as commission dyeing:",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":864,"listType":104,"direction":34},[865,871,877,881,885,891],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":866,"direction":34},[867,869],{"mode":31,"text":868,"type":33,"style":23,"detail":24,"format":6,"version":6},"The full route",{"mode":31,"text":870,"type":33,"style":23,"detail":24,"format":24,"version":6}," — pretreatment (desizing\u002Fscouring), dyeing, finishing and a colour lab",{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":872,"direction":34},[873,875],{"mode":31,"text":874,"type":33,"style":23,"detail":24,"format":6,"version":6},"Both batch (jet) and continuous equipment",{"mode":31,"text":876,"type":33,"style":23,"detail":24,"format":24,"version":6},"; BCI's continuous route covers light to dark shades, which suits long-run uniform fabric",{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":878,"direction":34},[879],{"mode":31,"text":880,"type":33,"style":23,"detail":24,"format":24,"version":6},"Three QC checkpoints — greige inspection before dyeing, in-process control and inspection at packing — with a 10-point system quality report",{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":882,"direction":34},[883],{"mode":31,"text":884,"type":33,"style":23,"detail":24,"format":6,"version":6},"Testing to ISO, JIS, AATCC and Daimaru methods",{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":886,"direction":34},[887,889],{"mode":31,"text":888,"type":33,"style":23,"detail":24,"format":6,"version":6},"OEKO-TEX Standard 100 certification",{"mode":31,"text":890,"type":33,"style":23,"detail":24,"format":24,"version":6}," — no restricted substances in the finished fabric",{"type":77,"value":199,"format":23,"indent":24,"version":6,"children":892,"direction":34},[893,895],{"mode":31,"text":894,"type":33,"style":23,"detail":24,"format":6,"version":6},"MOQ is negotiable",{"mode":31,"text":896,"type":33,"style":23,"detail":24,"format":24,"version":6}," — it depends on process, shade and order size",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":898,"direction":34},[899],{"mode":31,"text":900,"type":33,"style":23,"detail":24,"format":24,"version":6},"Q&A",{"type":36,"format":23,"indent":24,"version":6,"children":902,"direction":34,"textStyle":23,"textFormat":24},[903,905],{"mode":31,"text":904,"type":33,"style":23,"detail":24,"format":6,"version":6},"Q: Can TR be dyed with a single dye class?",{"mode":31,"text":906,"type":33,"style":23,"detail":24,"format":24,"version":6}," A: No. The polyester takes disperse dyes (high heat) and the rayon takes reactive or vat dyes. One class leaves the other fibre undyed.",{"type":36,"format":23,"indent":24,"version":6,"children":908,"direction":34,"textStyle":23,"textFormat":24},[909],{"mode":31,"text":910,"type":33,"style":23,"detail":24,"format":24,"version":6},"Q: How is TR different from TC, and which should I choose? A: TR uses rayon instead of cotton — softer, smoother and more absorbent, but with slightly lower wet strength and more shrinkage. TC suits work where durability and firmness matter; TR suits work where a soft, neat hand is wanted. BCI dyes both.",{"type":36,"format":23,"indent":24,"version":6,"children":912,"direction":34,"textStyle":23,"textFormat":24},[913,915],{"mode":31,"text":914,"type":33,"style":23,"detail":24,"format":6,"version":6},"Q: Why is the polyester dyed before the rayon?",{"mode":31,"text":916,"type":33,"style":23,"detail":24,"format":24,"version":6}," A: The disperse step runs at very high heat (130°C, or 180–220°C thermosol). If the reactive side were dyed first, that heat would destroy the reactive dyes — so the order is disperse first.",{"type":36,"format":23,"indent":24,"version":6,"children":918,"direction":34,"textStyle":23,"textFormat":24},[919,921],{"mode":31,"text":920,"type":33,"style":23,"detail":24,"format":6,"version":6},"Q: Why does TR shrink?",{"mode":31,"text":922,"type":33,"style":23,"detail":24,"format":24,"version":6}," A: Rayon (viscose) is more prone to shrinkage and shape loss than cotton, so TR needs finishing such as sanforizing to lock the dimensions before delivery.",{"type":36,"format":23,"indent":24,"version":6,"children":924,"direction":34,"textStyle":23,"textFormat":24},[925,927],{"mode":31,"text":926,"type":33,"style":23,"detail":24,"format":6,"version":6},"Q: What uniform work is TR best for?",{"mode":31,"text":928,"type":33,"style":23,"detail":24,"format":24,"version":6}," A: Office, hotel and work uniforms that need a soft, neat, comfortable hand while still standing up to frequent washing — BCI dyes TR for exactly this group.",{"type":36,"format":23,"indent":24,"version":6,"children":930,"direction":34,"textStyle":23,"textFormat":24},[931,933],{"mode":31,"text":932,"type":33,"style":23,"detail":24,"format":6,"version":6},"Q: Can small quantities of TR be dyed?",{"mode":31,"text":934,"type":33,"style":23,"detail":24,"format":24,"version":6}," A: MOQ is negotiable — it depends on process, shade and size; small runs can go on the batch (jet) route.",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":936,"direction":34},[937],{"mode":31,"text":938,"type":33,"style":23,"detail":24,"format":24,"version":6},"Talk to BCI",{"type":36,"format":23,"indent":24,"version":6,"children":940,"direction":34,"textStyle":23,"textFormat":24},[941,947,948,954,955],{"type":114,"fields":942,"format":23,"indent":24,"version":91,"children":944,"direction":34},{"url":943,"newTab":117,"linkType":118},"\u002Ffabric-dyeing\u002F",[945],{"mode":31,"text":946,"type":33,"style":23,"detail":24,"format":24,"version":6},"Commission TR fabric dyeing from the mill",{"mode":31,"text":460,"type":33,"style":23,"detail":24,"format":24,"version":6},{"type":114,"fields":949,"format":23,"indent":24,"version":91,"children":951,"direction":34},{"url":950,"newTab":117,"linkType":118},"\u002Funiform-fabrics\u002F",[952],{"mode":31,"text":953,"type":33,"style":23,"detail":24,"format":24,"version":6},"Uniform fabrics",{"mode":31,"text":460,"type":33,"style":23,"detail":24,"format":24,"version":6},{"type":114,"fields":956,"format":23,"indent":24,"version":91,"children":958,"direction":34},{"url":957,"newTab":117,"linkType":118},"\u002Fcontact-us\u002F",[959],{"mode":31,"text":960,"type":33,"style":23,"detail":24,"format":24,"version":6},"Contact the team",{"tag":27,"type":28,"format":23,"indent":24,"version":6,"children":962,"direction":34},[963],{"mode":31,"text":964,"type":33,"style":23,"detail":24,"format":24,"version":6},"References",{"tag":73,"type":74,"start":6,"format":23,"indent":24,"version":6,"children":966,"listType":104,"direction":34},[967,973,979,985,991],{"type":77,"value":6,"format":23,"indent":24,"version":6,"children":968,"direction":34},[969],{"type":114,"fields":970,"format":23,"indent":24,"version":91,"children":971,"direction":34},{"url":485,"newTab":486,"linkType":118},[972],{"mode":31,"text":489,"type":33,"style":23,"detail":24,"format":24,"version":6},{"type":77,"value":84,"format":23,"indent":24,"version":6,"children":974,"direction":34},[975],{"type":114,"fields":976,"format":23,"indent":24,"version":91,"children":977,"direction":34},{"url":494,"newTab":486,"linkType":118},[978],{"mode":31,"text":497,"type":33,"style":23,"detail":24,"format":24,"version":6},{"type":77,"value":91,"format":23,"indent":24,"version":6,"children":980,"direction":34},[981],{"type":114,"fields":982,"format":23,"indent":24,"version":91,"children":983,"direction":34},{"url":502,"newTab":486,"linkType":118},[984],{"mode":31,"text":505,"type":33,"style":23,"detail":24,"format":24,"version":6},{"type":77,"value":98,"format":23,"indent":24,"version":6,"children":986,"direction":34},[987],{"type":114,"fields":988,"format":23,"indent":24,"version":91,"children":989,"direction":34},{"url":510,"newTab":486,"linkType":118},[990],{"mode":31,"text":513,"type":33,"style":23,"detail":24,"format":24,"version":6},{"type":77,"value":192,"format":23,"indent":24,"version":6,"children":992,"direction":34},[993],{"type":114,"fields":994,"format":23,"indent":24,"version":91,"children":995,"direction":34},{"url":518,"newTab":486,"linkType":118},[996],{"mode":31,"text":521,"type":33,"style":23,"detail":24,"format":24,"version":6},"TR (polyester-rayon) fabric takes two dye systems: disperse for the polyester, reactive for the rayon. Process, fibre traits and why TR suits uniforms.","poly viscose fabric, polyester rayon blend dyeing, TR uniform fabric, TR fabric dyeing",{"id":1000,"alt":1001,"credit":1002,"updatedAt":1003,"createdAt":1003,"url":1004,"thumbnailURL":1002,"filename":1005,"mimeType":1006,"filesize":1007,"width":1008,"height":1009,"focalX":1010,"focalY":1010,"sizes":1011},117,"Stacked rolls of evenly dyed navy polyester-rayon uniform fabric in a textile mill",null,"2026-11-16T18:58:17.822Z","https:\u002F\u002Fpayload.bcg-app.com\u002Fapi\u002Fmedia\u002Ffile\u002Fdyeing-tr-fabric.webp","dyeing-tr-fabric.webp","image\u002Fwebp",36546,1024,576,50,{"card":1012,"hero":1018},{"url":1013,"width":1014,"height":1015,"mimeType":1006,"filesize":1016,"filename":1017},"https:\u002F\u002Fpayload.bcg-app.com\u002Fapi\u002Fmedia\u002Ffile\u002Fdyeing-tr-fabric-800x450.webp",800,450,16644,"dyeing-tr-fabric-800x450.webp",{"url":1002,"width":1002,"height":1002,"mimeType":1002,"filesize":1002,"filename":1002},"\u003Ch2>คำตอบสั้น: ผ้า TR ย้อมอย่างไร\u003C\u002Fh2>\u003Cp>ผ้า TR (polyester-rayon) คือผ้าผสมระหว่าง\u003Cstrong>โพลีเอสเตอร์กับเรยอง (วิสโคส)\u003C\u002Fstrong> ซึ่งเป็นเส้นใยเซลลูโลสที่นำกลับมาผลิตใหม่จากเยื่อไม้ — เพราะผืนเดียวมีเส้นใย 2 ชนิด จึง\u003Cstrong>ย้อมด้วยสีย้อมกลุ่มเดียวไม่ได้\u003C\u002Fstrong>: โพลีเอสเตอร์ใช้สีย้อมดิสเปอร์ส (ย้อมด้วยความร้อนสูง) ส่วนเรยองใช้สีย้อมรีแอคทีฟ (หรือ vat) ที่อุณหภูมิต่ำกว่า การย้อม 2 ระบบเรียงลำดับนี้เองที่ทำให้ผ้า TR มีทั้ง\u003Cstrong>ความนุ่มและทิ้งตัว (drape) ของเรยอง\u003C\u002Fstrong> และ\u003Cstrong>ทรงตัว ไม่หดง่ายของโพลีเอสเตอร์\u003C\u002Fstrong> ในผืนเดียว\u003C\u002Fp>\u003Ch2>ผ้า TR คืออะไร ต่างจากผ้า TC อย่างไร\u003C\u002Fh2>\u003Cp>TR คือผ้าผสม\u003Cstrong>โพลีเอสเตอร์ (T) กับเรยอง\u002Fวิสโคส (R)\u003C\u002Fstrong> — โครงสร้างการย้อมเหมือนผ้า TC ทุกประการ (2 ใย 2 สีย้อม) แต่เปลี่ยนเส้นใยด้านเซลลูโลสจาก\u003Cstrong>ฝ้ายเป็นเรยอง\u003C\u002Fstrong> ผลที่ตามมาคือ:\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>เรยองดูดน้ำและให้ความนุ่มมากกว่าฝ้าย\u003C\u002Fstrong> — เนื้อผ้าจึงนุ่ม เรียบ และทิ้งตัว (drape) กว่า TC\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>เรยองมีความแข็งแรงต่ำเมื่อเปียก\u003C\u002Fstrong> (wet strength ต่ำ) — ใช้น้ำหนักและความทนในการซัก-รีดที่เบากว่า TC เล็กน้อย\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Cstrong>เรยองหดตัวได้ง่ายกว่าฝ้าย\u003C\u002Fstrong> — ต้องอาศัยขั้นตอนหลังการย้อม (sanforize) คุมขนาดให้แน่นกว่า\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>เรยองติดสีได้สดใส\u003C\u002Fstrong> (amorphous region มาก) — เฉดสีจึงลึกและสดใส\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>ทำไมผ้า TR ต้องย้อม 2 ระบบ\u003C\u002Fh2>\u003Cp>ผืนเดียวมีเส้นใย 2 ชนิดที่เคมีต่างกัน จึงต้องใช้สีย้อมคนละกลุ่ม (กลไกเดียวกับผ้า TC — อ่านเพิ่มใน \u003Ca href=\"\u002Fth\u002Farticles\u002Fdyeing-tc-fabric\u002F\">ผ้า TC ย้อมอย่างไร\u003C\u002Fa>):\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>โพลีเอสเตอร์\u003C\u002Fstrong> — ไม่ดูดน้ำ ใช้\u003Cstrong>สีย้อมดิสเปอร์ส\u003C\u002Fstrong>: โมเลกุลเล็กซึมเข้าเส้นใยที่อุณหภูมิสูง (HTHP jet ราว 130°C หรือแบบต่อเนื่อง thermosol 180–220°C) — ดิสเปอร์สยึดกับโพลีเอสเตอร์เป็นหลัก ไม่ติดเส้นใยเซลลูโลส\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>เรยอง (เซลลูโลส)\u003C\u002Fstrong> — ใช้\u003Cstrong>สีย้อมรีแอคทีฟ\u003C\u002Fstrong> (สร้างพันธะเคมีกับเซลลูโลสที่ 60–80°C แล้วตรึงด้วยด่าง) หรือ\u003Cstrong>vat dye\u003C\u002Fstrong>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >ลำดับต้อง\u003Cstrong>ย้อมโพลีเอสเตอร์ก่อน\u003C\u002Fstrong> เพราะขั้นตอนดิสเปอร์สใช้ความร้อนสูงมาก — ถ้าย้อมรีแอคทีฟก่อน ความร้อนจากขั้นดิสเปอร์สจะทำลายสีย้อมรีแอคทีฟ\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>ขั้นตอนการย้อมผ้า TR\u003C\u002Fh2>\u003Col class=\"list-number\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>เตรียมผ้า (pretreatment)\u003C\u002Fstrong> — ฟอกแป้ง (desizing) ต้มฟอก (scouring) และฟอกขาวตามความจำเป็น; โพลีเอสเตอร์ต้อง\u003Cstrong>รีดร้อน (heat set)\u003C\u002Fstrong> ก่อน ไม่งั้นเส้นใยจะคลายตัวทำให้ผ้าเสียทรง\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>ย้อมโพลีเอสเตอร์\u003C\u002Fstrong> — สีย้อมดิสเปอร์ส ใน pH กรดอ่อน (ราว 5–6) ใช้น้ำยากระจายสีและสาร levelling ในเครื่อง jet (HTHP) หรือแบบต่อเนื่อง thermosol (จุ่มสีแล้วอบแห้ง 180–220°C)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Cstrong>ขจัดสีดิสเปอร์สที่เปื้อนเรยอง (reduction clearing)\u003C\u002Fstrong> — ล้างสีย้อมดิสเปอร์สที่เกาะเส้นใยเรยองออกก่อนย้อมขั้นถัดไป (ใช้เมื่อเฉดทำให้ด้านเรยองติดสี)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>ย้อมเรยอง\u003C\u002Fstrong> — สีย้อมรีแอคทีฟ (jet หรือ pad-batch) ที่ 60–80°C แล้วตรึงด้วยด่าง\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Cstrong>รีดสี (soaping) และล้าง\u003C\u002Fstrong> — ขจัดสีย้อมที่ยังไม่ตรึงออกด้วยความร้อนพร้อมผงซักฟอก แล้วล้างและอบแห้ง\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"6\"\n        >\u003Cstrong>หลังการย้อม (finishing)\u003C\u002Fstrong> — โดยเฉพาะ\u003Cstrong>กันหด (sanforizing)\u003C\u002Fstrong> เพื่อให้ผ้ายืนยันทรงสุดท้าย ซึ่งสำคัญมากสำหรับ TR\u003C\u002Fli>\u003C\u002Fol>\u003Ch2>ทำไมผ้า TR ถึงเหมาะกับการทำยูนิฟอร์ม\u003C\u002Fh2>\u003Cp>ยูนิฟอร์มต้องการผ้าที่\u003Cstrong>ดูเรียบร้อย นุ่ม สวมใส่สบาย และทนต่อการซัก-รีดบ่อย\u003C\u002Fstrong> — TR ตอบครบ:\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>เรยอง\u003C\u002Fstrong> ให้ความ\u003Cstrong>นุ่ม เรียบ ทิ้งตัว\u003C\u002Fstrong> และ\u003Cstrong>ดูดซับเหงื่อ\u003C\u002Fstrong> (moisture regain สูงกว่าฝ้าย) — สวมใส่สบาย\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>โพลีเอสเตอร์\u003C\u002Fstrong> ให้ความ\u003Cstrong>ทรงตัว ไม่หดง่าย ไม่ยับง่าย\u003C\u002Fstrong> และ\u003Cstrong>รีดง่าย\u003C\u002Fstrong>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >ผสมกันจึงได้ผ้ายูนิฟอร์มที่\u003Cstrong>นุ่มกว่า TC\u003C\u002Fstrong> แต่ยัง\u003Cstrong>ทนการซักบ่อย\u003C\u002Fstrong> — เหมาะกับชุดสำนักงาน โรงแรม และชุดทำงาน\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >เป็นผ้า\u003Cstrong>น้ำหนักมาตรฐานไปจนถึงหนา\u003C\u002Fstrong> (ไม่ใช่ผ้าบางเบา) ซึ่งเหมาะกับงานยูนิฟอร์มที่ต้องการความเรียบร้อย\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>เปรียบเทียบผ้า TR vs TC\u003C\u002Fh2>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>เส้นใยด้านเซลลูโลส\u003C\u002Fstrong>: TR = เรยอง (วิสโคส) \u002F TC = ฝ้าย\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>สัมผัส (hand)\u003C\u002Fstrong>: TR นุ่มและเรียบกว่า TC \u002F TC หนาและแข็งแรงกว่า\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Cstrong>การดูดซับ\u003C\u002Fstrong>: TR (เรยอง) ดูดน้ำและเหงื่อมากกว่าฝ้ายใน TC\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>ความแข็งแรงเมื่อเปียก (wet strength)\u003C\u002Fstrong>: TR ต่ำกว่า TC เล็กน้อย — เพราะเรยองอ่อนกว่าฝ้ายเมื่อเปียก\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Cstrong>การหดตัว\u003C\u002Fstrong>: TR (เรยอง) หดง่ายกว่า — ต้อง sanforize คุมแน่นกว่า\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"6\"\n        >\u003Cstrong>การใช้งานหลัก\u003C\u002Fstrong>: TR = ยูนิฟอร์มที่ต้องการความนุ่มเรียบร้อย \u002F TC = ยูนิฟอร์มที่ต้องการความทนและแข็งแรง\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>โรงงานย้อมผ้าคุมคุณภาพผ้า TR อย่างไร\u003C\u002Fh2>\u003Cp>เพราะ TR มีเส้นใย 2 ชนิด ควบคุมให้ได้สีเดียวและทรงตัวดีต้องอาศัย:\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>ห้องสี (colour lab)\u003C\u002Fstrong> — สเปกโทรโฟโตมิเตอร์ + ห้องตรวจสีหลายแหล่งแสง สำหรับทำ swatch (lab dip)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>ย้อมตัวอย่าง (lab dyeing) ที่จำลอง process ผลิตจริง\u003C\u002Fstrong> (batch และ continuous)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Cstrong>standard sample ที่ buyer ลงนาม\u003C\u002Fstrong> เก็บไว้เทียบข้ามออเดอร์\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>สูตรสีและ process conditions ที่ล็อกให้คงที่\u003C\u002Fstrong>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Cstrong>ค่า ΔE จากสเปกโทรโฟโตมิเตอร์\u003C\u002Fstrong> วัดความต่างสีของทุกล็อตเทียบกับ standard\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"6\"\n        >\u003Cstrong>การทดสอบตามมาตรฐานที่ระบุวิธีและระดับ\u003C\u002Fstrong> — เช่น ซัก (ISO 105-C06), สีติด (ISO 105-X12), แสง (ISO 105-B02), หดตัว (ISO 6330 \u002F AATCC 135)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"7\"\n        >รายงานคุณภาพระบบ 10 จุดทุกล็อต\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>บุญช่วยอุตสาหกรรม: รับย้อมผ้า TR\u003C\u002Fh2>\u003Cp>บุญช่วยอุตสาหกรรม (BCI) คือโรงงานฟอกย้อมและตกแต่งผ้าที่มีประสบการณ์\u003Cstrong>กว่า 60 ปี\u003C\u002Fstrong> ที่จังหวัดนครปฐม — \u003Cstrong>รับย้อมผ้า\u003C\u002Fstrong> กลุ่ม TR (โพลีเอสเตอร์-เรยอง) และ TC ซึ่งเป็นเส้นใยหลักของงานยูนิฟอร์ม:\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>process ครบ\u003C\u002Fstrong> — เตรียมผ้า (ฟอก\u002Fต้มฟอก), ย้อม, หลังการย้อม และห้องสี\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>เครื่องย้อมทั้ง batch (jet) และ continuous\u003C\u002Fstrong> — continuous ของ BCI ครอบคลุมสีอ่อนถึงเข้ม เหมาะกับออเดอร์ผ้ายูนิฟอร์มระยะยาว\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >QC 3 จุด — ตรวจผ้าดิบก่อนย้อม ควบคุมระหว่างกระบวนการ และตรวจตอนบรรจุ พร้อมรายงานคุณภาพระบบ 10 จุด\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>ทดสอบตามมาตรฐาน ISO, JIS, AATCC, Daimaru\u003C\u002Fstrong>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Cstrong>ใบรับรอง OEKO-TEX Standard 100\u003C\u002Fstrong> — ไม่มีสารห้ามใช้ในผ้าสำเร็จ\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"6\"\n        >\u003Cstrong>MOQ เจรจาได้\u003C\u002Fstrong> — ขึ้นกับ process, สี และขนาดออเดอร์\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>ถาม-ตอบ (FAQ)\u003C\u002Fh2>\u003Cp>\u003Cstrong>ถาม: ผ้า TR ย้อมด้วยสีย้อมกลุ่มเดียวได้ไหม?\u003C\u002Fstrong> ตอบ: ไม่ได้ — โพลีเอสเตอร์ต้องใช้สีย้อมดิสเปอร์ส (ความร้อนสูง) ส่วนเรยองใช้สีย้อมรีแอคทีฟหรือ vat ย้อมด้วยกลุ่มเดียวอีกเส้นใยจึงไม่ติดสี\u003C\u002Fp>\u003Cp>ถาม: TR กับ TC ต่างกันตรงไหน และควรเลือกอะไร? ตอบ: TR ใช้เรยองแทนฝ้าย — นุ่ม เรียบ และดูดซับมากกว่า แต่ความแข็งแรงตอนเปียกต่ำกว่าเล็กน้อยและหดง่ายกว่า TC เหมาะกับงานที่ต้องการความทนแข็งแรง TR เหมาะกับงานที่ต้องการความนุ่มเรียบร้อย BCI ย้อมได้ทั้งสอง\u003C\u002Fp>\u003Cp>\u003Cstrong>ถาม: ทำไมต้องย้อมโพลีเอสเตอร์ก่อนเรยอง?\u003C\u002Fstrong> ตอบ: ขั้นตอนดิสเปอร์สใช้ความร้อนสูงมาก (130°C หรือ thermosol 180–220°C) ถ้าย้อมรีแอคทีฟก่อน ความร้อนนั้นจะทำลายสีย้อมรีแอคทีฟจึงต้องเรียงลำดับดิสเปอร์สก่อน\u003C\u002Fp>\u003Cp>\u003Cstrong>ถาม: ทำไมผ้า TR ถึงหดตัว?\u003C\u002Fstrong> ตอบ: เรยอง (วิสโคส) มีแนวโน้มหดตัวและเสียทรงได้ง่ายกว่าฝ้าย จึงต้องอาศัยขั้นตอนหลังการย้อม เช่น sanforizing เพื่อล็อกขนาดให้แน่นก่อนส่งมอบ\u003C\u002Fp>\u003Cp>\u003Cstrong>ถาม: ผ้า TR เหมาะกับงานยูนิฟอร์มประเภทไหน?\u003C\u002Fstrong> ตอบ: ชุดสำนักงาน ชุดโรงแรม และชุดทำงานที่เน้นความนุ่ม เรียบ และสวมใส่สบาย ในขณะที่ยังต้องทนต่อการซัก-รีดบ่อย — BCI ย้อม TR สำหรับงานกลุ่มนี้\u003C\u002Fp>\u003Cp>\u003Cstrong>ถาม: จำนวนน้อยย้อม TR ได้ไหม?\u003C\u002Fstrong> ตอบ: MOQ เจรจาได้ — ขึ้นกับ process, สี และขนาด ล็อตเล็กสามารถเดินเครื่อง batch (jet) ได้\u003C\u002Fp>\u003Ch2>คุยกับทีม BCI\u003C\u002Fh2>\u003Cp>ดู \u003Ca href=\"\u002Fth\u002Ffabric-dyeing\u002F\">รับย้อมผ้า TR จากโรงงานย้อมผ้า\u003C\u002Fa> · \u003Ca href=\"\u002Fth\u002Funiform-fabrics\u002F\">ผ้ายูนิฟอร์ม\u003C\u002Fa> · หรือ \u003Ca href=\"\u002Fth\u002Fcontact-us\u002F\">สอบถาม\u003C\u002Fa>\u003C\u002Fp>\u003Ch2>แหล่งอ้างอิง\u003C\u002Fh2>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Ca href=\"https:\u002F\u002Ftextilelearner.net\u002Fproperties-of-viscose-rayon\u002F\" rel=\"noopener noreferrer\" target=\"_blank\">Physical, Chemical and Mechanical Properties of Viscose Rayon — Textile Learner\u003C\u002Fa>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Ca href=\"https:\u002F\u002Fskychemi.com\u002Fdisperse-dye-exhaust-vs-continuous-dyeing\u002F\" rel=\"noopener noreferrer\" target=\"_blank\">Disperse Dye Exhaust vs. Continuous Dyeing: A Process Guide for Polyester — Skychemi\u003C\u002Fa>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Ca href=\"https:\u002F\u002Fdaiwaborayon.co.jp\u002Fenglish\u002Ffeatures\" rel=\"noopener noreferrer\" target=\"_blank\">Characteristics of Viscose Rayon — Daiwabo Rayon Co., Ltd.\u003C\u002Fa>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Ca href=\"https:\u002F\u002Fwww.aatcc.org\u002Fwp-content\u002Fuploads\u002Fgibson_121979_18.pdf\" rel=\"noopener noreferrer\" target=\"_blank\">The Thermosol Story — Joseph W. Gibson Jr. (Olney Medal Address), AATCC\u003C\u002Fa>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Ca href=\"https:\u002F\u002Fwww.aatcc.org\u002Ftesting\u002Fstandards\" rel=\"noopener noreferrer\" target=\"_blank\">Standard Test Methods and Procedures — AATCC\u003C\u002Fa>\u003C\u002Fli>\u003C\u002Ful>","\u003Ch2>Short answer: how is TR fabric dyed\u003C\u002Fh2>\u003Cp>TR (polyester-rayon) fabric is a blend of \u003Cstrong>polyester and rayon (viscose)\u003C\u002Fstrong> — a regenerated cellulosic fibre made from wood pulp. Because one fabric carries two fibres, it \u003Cstrong>cannot be dyed with a single dye class\u003C\u002Fstrong>: the polyester takes \u003Cstrong>disperse dyes\u003C\u002Fstrong> (dyed at high heat) and the rayon takes \u003Cstrong>reactive (or vat) dyes\u003C\u002Fstrong> at a milder temperature. Running those two dye systems in sequence is what gives TR both the \u003Cstrong>softness and drape of rayon\u003C\u002Fstrong> and the \u003Cstrong>shape retention and low shrinkage of polyester\u003C\u002Fstrong> in a single fabric.\u003C\u002Fp>\u003Ch2>What TR is — and how it differs from TC\u003C\u002Fh2>\u003Cp>TR is a blend of \u003Cstrong>polyester (T) and rayon\u002Fviscose (R)\u003C\u002Fstrong>. Its dyeing structure is identical to TC (two fibres, two dye classes), but it swaps the cellulosic fibre from \u003Cstrong>cotton to rayon\u003C\u002Fstrong>. The consequences:\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>Rayon absorbs more water and is softer than cotton\u003C\u002Fstrong> — so TR has a softer, smoother, more draping hand than TC\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>Rayon has lower wet strength\u003C\u002Fstrong> — it handles slightly less well under heavy wash-and-wear than TC\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Cstrong>Rayon shrinks more readily than cotton\u003C\u002Fstrong> — so it needs tighter control in finishing (sanforizing)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>Rayon takes dye brightly\u003C\u002Fstrong> (more amorphous region) — so shades run deeper and more vivid\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>Why TR needs two dye systems\u003C\u002Fh2>\u003Cp>One fabric, two chemically different fibres, so two dye classes are required (the same mechanism as TC — see \u003Ca href=\"\u002Farticles\u002Fdyeing-tc-fabric\u002F\">How TC Fabric Is Dyed\u003C\u002Fa>):\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>Polyester\u003C\u002Fstrong> — hydrophobic; takes \u003Cstrong>disperse dyes\u003C\u002Fstrong>, whose small molecules enter the fibre at high temperature (HTHP jet around 130°C, or continuous thermosol at 180–220°C) — disperse bonds to polyester mainly and not to cellulosic fibres\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>Rayon (cellulosic)\u003C\u002Fstrong> — takes \u003Cstrong>reactive dyes\u003C\u002Fstrong> (a chemical bond to cellulose at 60–80°C, fixed with alkali) or \u003Cstrong>vat dyes\u003C\u002Fstrong>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >The order matters: \u003Cstrong>polyester is dyed first\u003C\u002Fstrong>, because the disperse step uses very high heat — dyeing the reactive side first would destroy the reactive dyes\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>How TR fabric is dyed, step by step\u003C\u002Fh2>\u003Col class=\"list-number\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>Pretreatment\u003C\u002Fstrong> — desizing, scouring, and bleaching where needed; the polyester is \u003Cstrong>heat-set\u003C\u002Fstrong> first, or the fibre relaxes and the fabric loses its shape\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>Polyester dyeing\u003C\u002Fstrong> — disperse dyes at mildly acidic pH (about 5–6) with a dispersing agent and a levelling agent, in a jet (HTHP) or by continuous thermosol (padding then dry heat at 180–220°C)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Cstrong>Reduction clearing\u003C\u002Fstrong> — strips disperse-dye staining from the rayon side before the next step (used whenever the shade leaves the rayon stained)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>Rayon dyeing\u003C\u002Fstrong> — reactive dyes (jet or pad-batch) at 60–80°C, fixed with alkali\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Cstrong>Soaping and washing\u003C\u002Fstrong> — unreacted dye is washed out at heat with detergent, then rinse and dry\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"6\"\n        >\u003Cstrong>Finishing\u003C\u002Fstrong> — especially \u003Cstrong>shrinkproofing (sanforizing)\u003C\u002Fstrong> to lock in the final shape, which matters more for TR\u003C\u002Fli>\u003C\u002Fol>\u003Ch2>Why TR is well suited to uniforms\u003C\u002Fh2>\u003Cp>Uniforms need a fabric that \u003Cstrong>looks neat, feels soft, is comfortable, and stands up to frequent washing\u003C\u002Fstrong> — TR delivers all of it:\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>Rayon\u003C\u002Fstrong> gives a \u003Cstrong>soft, smooth, draping hand\u003C\u002Fstrong> and \u003Cstrong>good sweat absorbency\u003C\u002Fstrong> (higher moisture regain than cotton) — comfortable to wear\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>Polyester\u003C\u002Fstrong> gives \u003Cstrong>shape retention, low shrinkage, low wrinkling\u003C\u002Fstrong> and \u003Cstrong>easy ironing\u003C\u002Fstrong>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >Combined, TR is a \u003Cstrong>softer uniform fabric than TC\u003C\u002Fstrong> that still \u003Cstrong>holds up to repeated washing\u003C\u002Fstrong> — a fit for office, hotel and work uniforms\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >It comes in \u003Cstrong>standard-to-heavier weights\u003C\u002Fstrong> (not a lightweight fabric), which suits neat uniform work\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>TR vs TC, side by side\u003C\u002Fh2>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>Cellulosic fibre\u003C\u002Fstrong>: TR = rayon (viscose) \u002F TC = cotton\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>Hand\u003C\u002Fstrong>: TR is softer and smoother \u002F TC is fuller and firmer\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Cstrong>Absorbency\u003C\u002Fstrong>: TR (rayon) absorbs more water and sweat than the cotton in TC\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>Wet strength\u003C\u002Fstrong>: TR is slightly lower than TC — rayon is weaker than cotton when wet\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Cstrong>Shrinkage\u003C\u002Fstrong>: TR (rayon) shrinks more readily — it needs tighter sanforizing control\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"6\"\n        >\u003Cstrong>Typical use\u003C\u002Fstrong>: TR = uniforms where a soft, neat hand is wanted \u002F TC = uniforms where durability and firmness are wanted\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>How a dyeing mill keeps TR quality consistent\u003C\u002Fh2>\u003Cp>Because TR carries two fibres, holding one shade and a stable shape takes:\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>A colour lab\u003C\u002Fstrong> — spectrophotometer plus a multi-source light booth for lab dips\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>Lab dyeing that mirrors the production route\u003C\u002Fstrong> (batch and continuous)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Cstrong>A buyer-signed standard sample\u003C\u002Fstrong> held for inter-order comparison\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>A locked recipe and process conditions\u003C\u002Fstrong>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Cstrong>ΔE from the spectrophotometer\u003C\u002Fstrong> measuring every lot against the standard\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"6\"\n        >\u003Cstrong>Testing to named methods and levels\u003C\u002Fstrong> — e.g. wash (ISO 105-C06), crocking (ISO 105-X12), light (ISO 105-B02), dimensional change (ISO 6330 \u002F AATCC 135)\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"7\"\n        >A 10-point system quality report for every lot\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>Boonchuay Industrial (BCI): commission dyeing for TR\u003C\u002Fh2>\u003Cp>BCI (Boonchuay Industrial) is a fabric dyeing and finishing mill with \u003Cstrong>over 60 years\u003C\u002Fstrong> of experience in Nakhon Pathom, Thailand. It takes \u003Cstrong>TR (polyester-rayon) and TC\u003C\u002Fstrong> — its core uniform fibres — as commission dyeing:\u003C\u002Fp>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Cstrong>The full route\u003C\u002Fstrong> — pretreatment (desizing\u002Fscouring), dyeing, finishing and a colour lab\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Cstrong>Both batch (jet) and continuous equipment\u003C\u002Fstrong>; BCI&#39;s continuous route covers light to dark shades, which suits long-run uniform fabric\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >Three QC checkpoints — greige inspection before dyeing, in-process control and inspection at packing — with a 10-point system quality report\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Cstrong>Testing to ISO, JIS, AATCC and Daimaru methods\u003C\u002Fstrong>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Cstrong>OEKO-TEX Standard 100 certification\u003C\u002Fstrong> — no restricted substances in the finished fabric\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"6\"\n        >\u003Cstrong>MOQ is negotiable\u003C\u002Fstrong> — it depends on process, shade and order size\u003C\u002Fli>\u003C\u002Ful>\u003Ch2>Q&amp;A\u003C\u002Fh2>\u003Cp>\u003Cstrong>Q: Can TR be dyed with a single dye class?\u003C\u002Fstrong> A: No. The polyester takes disperse dyes (high heat) and the rayon takes reactive or vat dyes. One class leaves the other fibre undyed.\u003C\u002Fp>\u003Cp>Q: How is TR different from TC, and which should I choose? A: TR uses rayon instead of cotton — softer, smoother and more absorbent, but with slightly lower wet strength and more shrinkage. TC suits work where durability and firmness matter; TR suits work where a soft, neat hand is wanted. BCI dyes both.\u003C\u002Fp>\u003Cp>\u003Cstrong>Q: Why is the polyester dyed before the rayon?\u003C\u002Fstrong> A: The disperse step runs at very high heat (130°C, or 180–220°C thermosol). If the reactive side were dyed first, that heat would destroy the reactive dyes — so the order is disperse first.\u003C\u002Fp>\u003Cp>\u003Cstrong>Q: Why does TR shrink?\u003C\u002Fstrong> A: Rayon (viscose) is more prone to shrinkage and shape loss than cotton, so TR needs finishing such as sanforizing to lock the dimensions before delivery.\u003C\u002Fp>\u003Cp>\u003Cstrong>Q: What uniform work is TR best for?\u003C\u002Fstrong> A: Office, hotel and work uniforms that need a soft, neat, comfortable hand while still standing up to frequent washing — BCI dyes TR for exactly this group.\u003C\u002Fp>\u003Cp>\u003Cstrong>Q: Can small quantities of TR be dyed?\u003C\u002Fstrong> A: MOQ is negotiable — it depends on process, shade and size; small runs can go on the batch (jet) route.\u003C\u002Fp>\u003Ch2>Talk to BCI\u003C\u002Fh2>\u003Cp>\u003Ca href=\"\u002Ffabric-dyeing\u002F\">Commission TR fabric dyeing from the mill\u003C\u002Fa> · \u003Ca href=\"\u002Funiform-fabrics\u002F\">Uniform fabrics\u003C\u002Fa> · \u003Ca href=\"\u002Fcontact-us\u002F\">Contact the team\u003C\u002Fa>\u003C\u002Fp>\u003Ch2>References\u003C\u002Fh2>\u003Cul class=\"list-bullet\">\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"1\"\n        >\u003Ca href=\"https:\u002F\u002Ftextilelearner.net\u002Fproperties-of-viscose-rayon\u002F\" rel=\"noopener noreferrer\" target=\"_blank\">Physical, Chemical and Mechanical Properties of Viscose Rayon — Textile Learner\u003C\u002Fa>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"2\"\n        >\u003Ca href=\"https:\u002F\u002Fskychemi.com\u002Fdisperse-dye-exhaust-vs-continuous-dyeing\u002F\" rel=\"noopener noreferrer\" target=\"_blank\">Disperse Dye Exhaust vs. Continuous Dyeing: A Process Guide for Polyester — Skychemi\u003C\u002Fa>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"3\"\n        >\u003Ca href=\"https:\u002F\u002Fdaiwaborayon.co.jp\u002Fenglish\u002Ffeatures\" rel=\"noopener noreferrer\" target=\"_blank\">Characteristics of Viscose Rayon — Daiwabo Rayon Co., Ltd.\u003C\u002Fa>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"4\"\n        >\u003Ca href=\"https:\u002F\u002Fwww.aatcc.org\u002Fwp-content\u002Fuploads\u002Fgibson_121979_18.pdf\" rel=\"noopener noreferrer\" target=\"_blank\">The Thermosol Story — Joseph W. Gibson Jr. (Olney Medal Address), AATCC\u003C\u002Fa>\u003C\u002Fli>\u003Cli\n          class=\"\"\n          style=\"\"\n          value=\"5\"\n        >\u003Ca href=\"https:\u002F\u002Fwww.aatcc.org\u002Ftesting\u002Fstandards\" rel=\"noopener noreferrer\" target=\"_blank\">Standard Test Methods and Procedures — AATCC\u003C\u002Fa>\u003C\u002Fli>\u003C\u002Ful>","2026-11-16T20:38:18.369Z","2026-11-16T18:58:03.455Z",1794861591496]